Process Piping Coating Case Study
This process piping coating job started with a costly mistake. About 24 km of new pipe at a Florida power plant rusted within ten months. Si-COAT 579 CM fixed it, with no abrasive blasting.
Twenty years later, the coating thickness had not changed. That job is the basis of our 20 year service life benchmark for Si-COAT 579 CM, made by CSL Silicones.

The problem: rust in under ten months
The plant sits at De Bary, Florida, about 56 km from the Atlantic coast. It is hot, humid and salty there, and the sun shines over 3,000 hours a year. In 2001, the plant replaced about 24 km of carbon steel process piping, plus fittings and instruments.
The specification called for blasting to white metal and an inorganic zinc rich coating. However, the pipe shop applied an alkyd paint instead, and nobody caught it before installation. Within ten months, rust had broken out along nearly every metre of pipe. Worst of all were the welds, fittings and instrument connections.
Why the plant needed a different process piping coating
Repairs looked painful. The budget was tight, and spraying wasn’t allowed inside the running plant. On top of that, the utility wanted the plant to keep looking new. So the coating had to go on by roller, in as few coats as possible, over minimal preparation.
The utility’s own corrosion lab already had the answer. Its Florida Fence Test had shown Si-COAT 579 CM holding up on rusted, hand cleaned steel. As a result, the lead corrosion engineer chose it for the piping.
How the process piping coating went on
Because 579 CM bonds to tight rust as well as to blasted steel, nobody needed to blast the pipe. Instead, the crew water blasted most of it at about 345 bar (5,000 psi) with a turbo tip. Then they power tool cleaned the heavily rusted welds to SSPC SP3 and wiped them down with solvent.
Next, every weld got a spot prime of 579 CM itself, at 0.15 mm dry film (152 microns, 6 mil). Finally, the crew rolled one full coat over everything, at 0.23 mm (229 microns, 9 mil). The work ran from February to September 2003.
Skipping the blasting and the extra coats saved both material and labour, compared with a three coat epoxy and urethane system.
Twenty years later
About 20 years after the job, CSL went back and measured the coating. The thickness had not changed. In other words, two decades of Florida heat, humidity and UV had not worn it down.
That is why we quote a service life of about 20 years for Si-COAT 579 CM. We don’t stretch it further, because this is the longest record we can stand behind.
What this means for Southern African plants
Many plants here face the same trap: rusted pipe racks nobody can blast, in plants that can’t stop. For example, chemical plants, refineries and power stations often limit open blasting near live equipment. Similarly, coastal sites in Durban and Richards Bay deal with the same salt, heat and humidity as De Bary. In those plants, the right process piping coating has to go on over rust, by roller, in one coat.
For product details, see our silicone corrosion coating page. Also read about the Hoopstad fertiliser plant, the chlorine plant in Johannesburg and our guide to surface tolerant coating.